Nylon’s tendency to absorb moisture is perhaps the most important characteristic to understand when designing with this material. Proper design can turn this characteristic from a challenge into a manageable variable.
Why Does Nylon Absorb Water?
Nylon’s molecular structure contains polar amide groups (-CONH-) that form hydrogen bonds with water molecules, causing the material to absorb moisture from humid air or liquid water.
Moisture Absorption by Nylon Grade
| Nylon Grade | Moisture at 50% RH | Saturation in Water | Dimensional Change |
|---|---|---|---|
| PA6 | 2.5-3.0% | 9.5% | 0.5-1.0% |
| PA66 | 2.0-2.5% | 8.0% | 0.4-0.8% |
| PA11 | 0.8% | 1.9% | 0.1-0.3% |
| PA12 | 0.7% | 1.5% | 0.1-0.3% |
| PA6 GF30 | 1.7-2.1% | 6.5% | 0.2-0.4% |

How Moisture Affects Mechanical Properties
Water acts as a plasticizer within the nylon matrix. A PA6 part at 50% RH can lose 20-40% of dry tensile strength and 30-50% of dry flexural modulus.
Impact Resistance Increases

Moisture conditioning improves impact resistance by 2-3x. This is why nylon parts are frequently conditioned before use in impact-critical applications.
Design Strategies for Dimensional Control
- Use glass-filled grades: GF30 absorbs ~30% less moisture
- Select low-moisture grades: PA11/PA12 for critical applications
- Design clearances: Account for swelling in tolerance calculations
- Pre-condition parts: Condition before final machining
- Use symmetrical designs: Symmetrical parts swell more uniformly

Processing Implications
Before processing, nylon must be dried to <0.2% moisture. Insufficient drying results in splay marks, reduced mechanical properties, and inconsistent dimensions.
Drying Recommendations
| Grade | Drying Temp | Time | Target Moisture |
|---|---|---|---|
| PA6 | 80°C | 4-8 hrs | < 0.10% |
| PA66 | 80°C | 4-8 hrs | < 0.10% |
| PA12 | 80°C | 3-4 hrs | < 0.05% |
Nos compétences
Avec plus de 300 machines à commande numérique, nous produisons plus de 10 000 pièces par jour avec des tolérances aussi strictes que ±0,005 mm. Nous acceptons Quantité minimale de commande : à partir d'une pièce, avec des délais de livraison allant de De 24 heures à 15 jours. We understand nylon’s moisture behavior and design accordingly. Recevez un devis sous 24 heures.
FAQ
How do you know whether Understanding Nylon Water Absorption: Impact on Dimensional Stability and Performance fits a part?
Understanding Nylon Water Absorption: Impact on Dimensional Stability and Performance fits a part when its load capacity, temperature range, moisture exposure, wear behavior, and processing method match the real service conditions.
What properties should be checked for Understanding Nylon Water Absorption: Impact on Dimensional Stability and Performance?
Vérifier la résistance, la rigidité, la résistance aux chocs, la résistance à la chaleur, l'absorption d'humidité, la stabilité dimensionnelle, le frottement, l'usure et la compatibilité chimique.
What is the biggest selection risk for Understanding Nylon Water Absorption: Impact on Dimensional Stability and Performance?
Le plus grand risque est de choisir à partir d'une fiche technique sans tenir compte de l'environnement réel, de la méthode de traitement, de la géométrie de la pièce et de l'utilisation à long terme.
When should Understanding Nylon Water Absorption: Impact on Dimensional Stability and Performance be tested before production?
Les essais sont recommandés lorsque la pièce est soumise à une charge, à la chaleur, à des produits chimiques, à l'humidité, à des tolérances serrées, à des exigences réglementaires ou à un nouvel environnement de travail.